When Allegheny Ludlum developed AL-6XN® alloy (N08367), they intended to create an austenitic stainless alloy that could be made in all product forms and would have superior corrosion resistance properties. AL-6XN is the leading 6Mo stainless alloy due to its excellent chemical, corrosion resistant, mechanical, and high temperature properties.

Chemical Composition of AL-6XN Alloy

AL-6XN's outstanding resistance to corrosion is due to higher concentrations of the following elements:
  • Nitrogen – Slows the formation of chi phase during manufacturing and field welding
  • Chromium – Provides good resistance to oxidizing environments
  • Molybdenum – Improves resistance to chlorides
  • Nickel – Stabilizes the austenitic microstructure and improves overall general corrosion resistance
ElementUNS N08367
Carbon (C)0.03 maximum
Manganese (Mn)2.00 maximum
Phosphorus (P)0.040 maximum
Sulfur (S)0.030 maximum
Silicon (Si)1.00 maximum
Chromium (Cr)20.00 – 22.00
Nickel (Ni)23.50 – 25.50
Molybdenum (Mo)6.00 – 7.00
Nitrogen (Ni)0.18 – 0.25
Copper (Cu)0.75 maximum
Iron (Fe)Balance

ABOUT AL-6XN ALLOY

AL-6XN alloy has exceptional resistance to chloride corrosion, pitting, crevice corrosion, and stress corrosion cracking. It has excellent corrosion resistance to various acids, alkalis, and salt solutions.

Shop Now

Alloy Chemical Comparison

Super AusteniticDuplexTraditional
AL-6XN

(UNS N08367)

254 SMO

(UNS S31254)

904L

(UNS N08904)

2507

(UNS S32750)

2205

(UNS S32205)

1.4435

(UNS S31603)

316L

(UNS S31603)

% Carbon0.030 max.0.0200.0200.0300.03 max0.030 max0.030
% Chromium20.0-22.019.5-20.519.0-23.024.0-26.022.0-23.017.0 – 19.016.0 – 18.0
% Nickel23.5-25.517.5-18.523.0-28.06.0-8.04.5-6.512.5-15.010.0 – 14.0
% Molybdenum6.0-7.06.0-6.54.0- 5.03.0-5.03.0-3.52.5 – 3.02.0 – 3.0
% Nitrogen0.18-0.250.18-0.220.150.24-0.320.140.110.10
% Iron (Fe)48 Balance54 Balance47 BalanceBalanceBalanceBalanceBalance
% Manganese2.0 max.1.02.02.002.0 max2.0 max2.0
% Phosphorous0.040 max.0.0300.0450.0300.0300.045 max0.045
% Sulfur0.030 max.0.0100.0350.020.020.0250.030
% Silicon1.00 max.0.801.01.001.00 max1.00 max0.75
% Copper0.75 max.0.5-1.01.0-2.00.5-

Physical Properties of AL-6XN Alloy

Due to the stable, face-centered cubic crystal structure, commonly referred to as austenitic structure, AL-6XN alloy can be easily used in fabrication. AL-6XN alloy is a good alternative to titanium in condenser tubing applications, as a result of the excellent physical properties listed below.

PropertyValue
Density0.291lb/in3
8.06 g/cm3
Modulus of Elasticity28.3 x 106 psi
195 GPa
Melting Range2410 – 2550°F
1320 – 1400°C
Thermal Conductivity
68 – 212°F
20 – 100°C

6.8 Btu/hr • ft • °F
11.8 W/mK
Coefficient of Expansion
68 – 212°F
20 – 100°C

8.5 • 10-6/°F
15.3 • 10-6/°C
Specific Heat Capacity0.11 Btu/lb • °F
500 J/kg • K
Electrical Resistivity535 Ohm • circ mil/ft
0.89 µohm • cm
Magnetic Permeability
Fully annealed 0.5" plate
65% cold-worked plate

1.0028 Oersted
1.0028 (µ at 200H)
Scaling Temperature1885°F